Alloy 218 Forgings (UNS S21800) Seamless rolled rings, forged flanges, round bars, shafts, discs, sleeves, bushings and tube sheets to AMS 5848, ASTM A276 and ASTM A479

Alloy 218 is a nitrogen-strengthened austenitic stainless steel containing about 17 percent chromium, 8.5 percent nickel, 8 percent manganese and 4 percent silicon. The silicon and manganese additions give it resistance to galling, wear and fretting in the annealed condition, which is why it replaces 304 and 316 in valve stems, bridge pins, fasteners and bushings that seize in service.

UNS number
S21800
Other designations
Alloy 218, Nitronic 60
Alloy type
Austenitic, nitrogen strengthened
Tensile, annealed, min
95 ksi (655 MPa)
Yield 0.2 percent, min
50 ksi (345 MPa)
Hardness, solution treated
170 to 255 HB
Strength retained to
1800 F (982 C)
Main specifications
AMS 5848, ASTM A276, ASTM A479

Alloy 218, UNS S21800 and Nitronic 60

Enquiries and drawings use all three names for the same material. Nitronic is a registered trademark of its proprietor, so purchase orders and mill certificates normally carry the generic designations UNS S21800 or Alloy 218. A drawing calling for Nitronic 60 is quoted and certified here as UNS S21800 to AMS 5848 or ASTM A276, with no change to chemistry or properties.

Chemical composition

Composition limits in weight percent, to ASTM A276 and AMS 5848. Balance iron.
ElementMinMax
Carbon (C)–0.10
Chromium (Cr)16.018.0
Nickel (Ni)8.09.0
Manganese (Mn)7.09.0
Silicon (Si)3.54.5
Nitrogen (N)0.080.18
Molybdenum (Mo)–0.75
Phosphorus (P)–0.060
Sulfur (S)–0.030
Iron (Fe)Balance
Published phosphorus and sulfur limits vary. ASTM A276 is commonly listed as P 0.060 max and S 0.030 max, while some stockholders quote P 0.040 max and S 0.010 max. State the tighter limits on the enquiry if your specification requires them and the heat will be melted and certified to them.

Mechanical properties

Solution annealed

ASTM A276 minimum requirements for annealed product, with AMS 5848 solution-treated values by section size.
ConditionTensileYield, 0.2 percentElongation, 4DReduction of areaHardness
ASTM A276, annealed, minimum95 ksi (655 MPa)50 ksi (345 MPa)35 percent––
AMS 5848, under 0.5 in section105 ksi (724 MPa)55 ksi (379 MPa)35 percent55 percent170 to 255 HB
AMS 5848, over 0.5 in section95 ksi (655 MPa)50 ksi (345 MPa)35 percent55 percent170 to 255 HB
Forged rings, flanges, shafts and discs are nearly always thicker than 0.5 in (12.7 mm), so design and acceptance testing should use the 95 ksi tensile and 50 ksi yield row. Quoting the thin-section figures of 105 and 55 ksi on heavy forgings is a frequent cause of third-party retest rejection.

Strain hardened bar

Minimum values for cold-worked strength levels. Confirm against the current specification revision before ordering.
LevelDiameterTensile, minYield, minElongation, minReduction of area, min
HS 10.125 to 4.00 in110 ksi90 ksi35 percent55 percent
HS 20.125 to 4.00 in135 ksi105 ksi20 percent50 percent
HS 30.125 to 3.50 in160 ksi130 ksi15 percent45 percent
HS 40.062 to 2.00 in180 ksi145 ksi12 percent45 percent
HS 50.062 to 1.50 in200 ksi180 ksi10 percent45 percent

Cold work raises strength but does not improve the anti-galling behaviour. That property comes from the silicon and manganese chemistry and is already present in annealed material.

Physical properties

Typical room-temperature values for UNS S21800.
PropertyImperialMetric
Density0.275 lb/in³7.61 g/cm³
Modulus of elasticity26.2 x 10⁶ psi181 GPa
Thermal expansion, 68 to 212 F8.8 x 10⁻⁶ per F15.8 x 10⁻⁶ per C
Thermal conductivity9.0 Btu/ft·hr·Fabout 15.6 W/m·K
Specific heat0.12 Btu/lb·Fabout 502 J/kg·K
Electrical resistivity28.7 micro-ohm·inabout 72.9 micro-ohm·cm

Corrosion, oxidation and heat treatment

General corrosion

Resistance sits between 304 and 316 stainless steel. The alloy suits chemical process, marine and food contact duty where wear rather than aggressive chemistry is the limiting factor.

Oxidation

Similar to 309 stainless steel and better than 304, a result of the high silicon content.

Elevated temperature

Developed as a high-temperature alloy. It holds useful strength and galling resistance to about 1800 F (982 C).

Heat treatment

Not hardenable by heat treatment. Solution anneal at about 1950 F (1066 C) and water quench.

Where Alloy 218 forgings are used

Valves and flow control

Valve stems, seats and trim, valve bodies and seat rings, pump wear rings and lobes, gate valves on seawater ballast systems.

Bridges and construction

Bridge pins and pin and hanger expansion joints, specified over A36 and A588 carbon steel for galling resistance and low-temperature toughness.

Fasteners and sliding parts

Nuts, bolts and studs to ASTM A193 Grade B8S and ASTM A194, pins, bushings, roller bearings, chain drive parts and screens that are assembled and dismantled repeatedly.

Marine and subsea

Seawater pump shafts, boat shafting, deep-sea sampler and incubation chambers, underwater manipulator components.

Oil and gas

Down-hole and oil field production equipment, wellhead and christmas tree parts, compressor shafts, forged manifolds and nozzles.

Rotating equipment

Shafts and spindles, gear blanks and gearbox parts, turbine and gas compressor components, forged rolls and wheels.

Forged shapes and size range

Alloy 218 product forms produced at Jiangyin Jiangnan Metal.
FormSize rangeSupply condition
Seamless rolled ringsOD [min] to [max] mm, height to [max] mmSolution annealed, rough machined
Forged flanges and tube sheetsOD to [max] mmAnnealed, machined to drawing
Round bars, shafts and spindlesDiameter [min] to [max] mm, length to [max] mmAnnealed, peeled or turned
Discs, blanks and gear blanksDiameter to [max] mmAnnealed, rough machined
Sleeves, bushings and hollow forgingsOD to [max] mm, bore from [min] mmAnnealed, bored
Near-net open-die preformsPiece weight [min] to [max] kgAs forged and annealed

Melting, testing and certification

Alloy 218 is melted by AOD refining or vacuum induction melting. Vacuum arc remelting and electroslag remelting are available where cleanliness requirements call for them. Every forging is solution annealed and water quenched before final machining.

Ultrasonic examination follows EN 10228-3, SEP 1921 or ASTM A388 as stated on the order. Documentation covers chemical analysis, tensile and hardness results, positive material identification and a dimensional report. Certificates are issued to EN 10204 3.1, or to EN 10204 3.2 with third-party witness such as TUV, SGS, BV or Lloyd's Register. Charpy impact testing at sub-zero temperature and grain size checks are added on request.

Specifications and equivalents

CategoryReference
UNSS21800
Bars, wire and forgingsAMS 5848
Bars and shapesASTM A276, ASME SA276
Bars for pressure serviceASTM A479, ASME SA479
BoltingASTM A193 Grade B8S, ASTM A194, ASME SA194
Sheet and plateASTM A240
Trade and common namesAlloy 218, Nitronic 60

Questions buyers ask

Is Alloy 218 the same material as Nitronic 60?

Yes. Alloy 218, Nitronic 60 and UNS S21800 all describe the same nitrogen-strengthened austenitic stainless steel. Because Nitronic is a trademark, orders and certificates use Alloy 218 or UNS S21800.

Which strength values apply to a forged ring or shaft?

Use 95 ksi (655 MPa) minimum tensile, 50 ksi (345 MPa) minimum yield at 0.2 percent offset and 35 percent minimum elongation, with hardness of 170 to 255 HB. The higher 105 and 55 ksi figures in AMS 5848 apply only to sections under 0.5 in.

Can the alloy be hardened by heat treatment?

No. It is austenitic and non-hardenable. Strength is increased by cold work, with strain-hardened levels from 110 ksi up to 200 ksi minimum tensile. Galling resistance does not change with cold work.

How does corrosion resistance compare with 304, 316 and duplex grades?

General corrosion resistance falls between 304 and 316, and oxidation resistance is close to 309. Specify Alloy 218 when galling, wear and fretting govern. Where chloride pitting governs, a duplex or 6Mo grade such as A182-F51, A182-F55 or A182-F44 is the better choice.

What is the correct annealing cycle?

Solution anneal at about 1950 F (1066 C), then water quench. Avoid slow cooling through the sensitisation range.

How is Alloy 218 priced and what is the minimum order?

Forgings are made to order, so price depends on the drawing, the piece weight, the machining allowance and the quantity. There is no catalogue price. Orders start from a single prototype piece and run through to series production. Send the drawing, or the outside diameter, bore and height with the governing specification, and a written quotation follows within one working day.

Request a quotation for Alloy 218 forgings

Send the drawing, or the outside diameter, bore, height or length, the quantity and the governing specification such as AMS 5848, ASTM A276, ASTM A479 or ASTM A193 Grade B8S. The reply confirms the forging route, the test plan, the certificate package and the price.

Email sales@steelforgepieces.com Call 0086-189-2135-9659

Related grades produced here

Data sources: composition and mechanical requirements of ASTM A276, ASTM A479 and AMS 5848, together with producer data sheets for UNS S21800 covering annealing practice, physical properties and strain-hardened strength levels. Values are typical and given for guidance only. They do not replace the governing specification or a project design allowable. Data sheet revision: October 2026.

FactoryJiangyin Jiangnan Metal Co., Ltd.
Open-die forging factory
AddressNo.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province 214423, China
Telephone0086-189-2135-9659
Emailsales@steelforgepieces.com