GRADE X3CrNiMoAl13-8-2  /  W.NR 1.4534  /  UNS S13800 JIANGYIN JIANGNAN METAL  ·  +86 189 2135 9659  ·  sales@steelforgepieces.com
Jiangnan Metal Melting · Open-die forging · Ring rolling Get a price

Precipitation-hardening stainless steel

X3CrNiMoAl13-8-2 1.4534 · UNS S13800 · PH 13-8 Mo · ASTM XM-13 · AMS 5629

X3CrNiMoAl13-8-2 is a martensitic precipitation-hardening stainless steel with 12.25 to 13.25 per cent chromium, 7.5 to 8.5 per cent nickel, 2.0 to 2.5 per cent molybdenum and 0.90 to 1.35 per cent aluminium. It reaches 1515 MPa in the H950 condition yet keeps transverse toughness close to its longitudinal values, which is why designers choose it over other PH grades for thick forged sections in subsea, valve, aerospace and pump service.

Jiangyin Jiangnan Metal melts this grade on site and forges it in the same works. Sulphur is limited to 0.008 per cent and phosphorus to 0.010 per cent, so the heat is refined under vacuum and remelted by ESR or VAR rather than bought in as billet. Rings, shafts, flanges, discs and valve parts follow, solution treated and aged to the condition on your drawing.

Grade data sheet1.4534
Type
Martensitic PH stainless
Equivalents
UNS S13800 · PH 13-8 Mo · ASTM XM-13 · AMS 5629 · BS 13-8 · 04Cr13Ni8Mo2Al
Melt route
EF + LF + VOD, remelted by ESR or VAR. 60 t maximum heat
Conditions
A · RH950 · H950 · H1000 · H1025 · H1050 · H1100 · H1150 · H1150M
Strength
1515 MPa minimum tensile, 1415 MPa proof, 45 HRC in H950
Forms
Rolled rings, forged rings, shafts, flanges, bars, discs, sleeves, tube sheets, valve parts
Testing
UT to ASTM A388, EN 10228-3 or SEP 1921; MT to ASTM E709
Certificate
EN 10204 3.1 standard, 3.2 witnessed on request
Minimum
10 kg, no minimum piece count. Lead time 20 to 60 days
01

Designations and equivalents

The same alloy carries different names depending on the standard a drawing was written to. Any of the designations below can be quoted as X3CrNiMoAl13-8-2 forging stock.

Equivalent designations
Standard or systemDesignation
EN / WerkstoffX3CrNiMoAl13-8-2, 1.4534
UNSS13800
ASTMA564 XM-13, A693 XM-13, A705 XM-13, A959 XM-13
AMSAMS 5629
Trade namesPH 13-8 Mo, 13-8 Mo, Marval X12
BritishBS 13-8, N709
French (AFNOR)Z1CNDA12-09, Z4CNDAT13-09, X1CrNiMoAl12-9
Chinese04Cr13Ni8Mo2Al

Neighbouring grades forged in the same shop: PH 13-8 Mo, 17-4 PH, 17-7 PH and 15-5 PH.

02

Chemical composition

Sulphur at 0.008 per cent and phosphorus at 0.010 per cent are the limits that govern the melting route. They cannot be met by arc melting alone, which is why the grade is normally double melted. Aluminium is the hardening element: it forms the fine NiAl precipitate that gives the alloy its strength on ageing.

Composition, weight per cent. ASTM XM-13 and UNS S13800 limits, with EN 1.4534 variations
ElementMinimumMaximumEN 1.4534 variation
Carbon, C–0.05
Silicon, Si–0.10
Manganese, Mn–0.200.10 maximum
Phosphorus, P–0.010
Sulphur, S–0.008
Chromium, Cr12.2513.25
Nickel, Ni7.508.50
Molybdenum, Mo2.002.50
Aluminium, Al0.901.350.90 to 1.20
Nitrogen, N–0.010
Iron, FeBalance, about 76

Chemistry is checked at the furnace on a SPECTROTEST TXC25 optical emission spectrometer to ASTM E415, with carbon and sulphur confirmed on an infrared analyser to ASTM E1019. Because the steel is melted here, the certificate reports a melt analysis rather than repeating a billet supplier's figures.

03

Mechanical properties

Two tables follow. The first lists what the specification demands, the second what the material usually delivers. Order acceptance is always against the first.

Specified minima, ASTM A564 grade XM-13

Required room-temperature properties by condition
ConditionTensile, MPa0.2% proof, MPaElongation, %Hardness, HRCHardness, HB
A, solution treated–––38 max363 max
H950151514151045450
H1000141513101043400
H1025128012101141380
H1050121011401240372
H110010359501434313
H11509306201430283
H1150M8605851626259

Typical longitudinal values

Typical room-temperature properties including Charpy V-notch energy
Condition0.2% proof, MPaTensile, MPaElongation in 50 mm, %Reduction of area, %HRCCVN, J
RH9501482162012454827
H9501449155112504727
H10001413148213554541
H10501241131015554368
H11001034110318603581
H11507241000206333103
H1150M586896227032163

Transverse values stay close to longitudinal ones. In H950 a typical transverse test gives about 1448 MPa proof strength and 1551 MPa tensile at 12 per cent elongation, within a few MPa of the longitudinal figures. For a ring or a heavy disc, where the critical stress often runs across the grain flow, that is the property that decides the grade.

Tensile testing runs in house on a 600 kN WE-600B machine and a WDW-300 electronic machine to ASTM A370 and ISO 6892. Charpy impact testing uses a JBN-300 pendulum with a DWC-60 low-temperature bath, down to minus 60 degrees Celsius; tests below that are placed with an accredited laboratory.

04

Physical properties

Physical and thermal data
PropertyValueCondition or temperature
Density7.76 to 7.8 g/cm³H1000, room temperature
Modulus of elasticity195 to 203 GParoom temperature
Modulus of rigidity76.5 GPaH950
Poisson's ratio0.27 to 0.30room temperature
Thermal conductivity14 to 15 W/m·Kcondition A, 100 °C
Specific heat capacityabout 500 J/kg·K20 °C
Mean thermal expansion10.6 × 10-6 /KH950, 21 to 93 °C
Electrical resistivityabout 1020 µΩ·mmcondition A, 100 °C
Magnetic responseFerromagneticall conditions
Service temperaturehigh strength held to about 315 °C; oxidation resistance to about 595 °C–
Design note

Long exposure between roughly 288 and 482 degrees Celsius can lower toughness in precipitation-hardening stainless steels. Ageing at a higher temperature reduces the effect, and service excursions should stay at least 28 degrees below the ageing temperature used.

05

Heat treatment conditions

Solution treatment and ageing are carried out here, in 14 furnaces that include car-bottom chambers to 8,000 by 2,000 by 2,000 mm and two 15 m well-type furnaces for quenching long shafts vertically. Parts can leave in condition A for machining, or finished in the aged condition.

Treatment cycles for 1.4534 and UNS S13800
ConditionCycle
A927 °C ± 8 °C, hold to section, then cool below 16 °C to complete the transformation to martensite. Sections under about 230 cm² may be liquid quenched; heavier sections air cool.
RH950From condition A: hold at minus 73 °C for at least 2 hours within 24 hours of solution treatment, warm in air, then age at 510 °C ± 6 °C for 4 hours and air cool.
H950510 °C for 4 hours, air cool.
H1000538 °C for 4 hours, air cool.
H1025552 °C for 4 hours, air cool.
H1050566 °C for 4 hours, air cool.
H1100593 °C for 4 hours, air cool.
H1150621 °C for 4 hours, air cool.
H1150M760 °C for 2 hours, air cool, then 621 °C for 4 hours, air cool. Best machinability of the aged conditions.
Two traps worth avoiding

H900 belongs to 17-4 PH and does not exist for this grade; 510 °C, giving H950, is as low as the ageing goes. And material delivered in H1150 or H1150M will not respond to further ageing until it has been re-solution treated at 927 °C. Hardness alone will not tell the two apart, because the H1150 range overlaps the solution-treated range, so the heat-treatment record has to be read.

Ageing contracts the part by a predictable amount, roughly 0.0004 to 0.0006 mm per mm for H950 and H1000, 0.0005 to 0.0008 for H1050 and 0.0008 to 0.0012 for H1100. Machining allowances are set against the condition on the order.

06

Forging, machining and welding

Forging

Heat to between 1177 and 1204 degrees Celsius and soak for about an hour at temperature. Forging stops at 955 degrees; working below that risks cracking and leaves the grain structure uneven. Pieces are air cooled below about 16 degrees after forging, then solution treated before any ageing, so the material responds properly to precipitation hardening. Scale is removed by grit blasting or acid cleaning, and finished surfaces are passivated.

Machining

In condition A the grade cuts cleanly and holds a good finish, but at speeds roughly 20 to 30 per cent below 17-4 PH or type 302 and 304 stainless. Machinability improves as the ageing temperature rises, and H1150M is the easiest of the aged conditions. At H950 the material sits near 47 HRC, and turning, drilling and milling slow down accordingly. For parts with heavy machining content, the usual route is to supply in condition A or H1150M and age afterwards. Bars should be cold sawn rather than cut with an abrasive wheel, which can leave fine surface cracks on annealed stock.

Welding

Inert-gas shielded and resistance processes both work, normally on solution-annealed material with 13-8 Mo filler, and preheat is not usually needed. Where full weld strength is not required, E308L or ER308L consumables can be used. Sharp corners, threads and partial-penetration joints should be designed out. Solution treating the welded assembly before ageing gives the best combination of strength, ductility and corrosion resistance.

07

Corrosion behaviour

In the H950 condition the alloy resists rusting in 5 per cent salt fog about as well as type 304, and in oxidising and reducing acids and in open-air exposure its general corrosion resistance comes close to 304. Resistance is highest fully hardened and falls off slightly as the ageing temperature rises.

Marine-atmosphere testing shows a high level of resistance to stress-corrosion cracking in both wrought and welded material. For service where cracking is the governing risk, ageing at 538 degrees Celsius or above is the usual recommendation. The grade also behaves well against sodium chloride, nitric acid and sodium hydroxide. Surfaces must be free of scale and embedded iron, and finished parts should be passivated before shipment.

08

Forgings supplied in this grade

Everything below is forged from a single piece of steel melted on site. No welding, no casting, no purchased billet of unknown origin.

Product forms in X3CrNiMoAl13-8-2
FormDetail
Seamless rolled ringsRing-rolled from a punched preform on a radial-axial mill, rectangular or contoured section
Forged ringsUpset and punched, for sections outside the ring-mill envelope and where heavy reduction is wanted
Forged shafts and spindlesStepped, eccentric and crankshaft forms, quenched vertically in the well furnaces where length demands it
Forged flangesWeld neck, blind, slip-on, long weld neck and special profiles
Round bars, blocks and billetsPress forged with a recorded reduction ratio
Discs, tube sheets and coversUpset forged, solid or trepanned, proof-machined for volumetric inspection
Sleeves and bushingsBored on the deep-hole drilling machine, to 1,600 mm diameter by 10,000 mm
Forged pipes and hollow barsTrepanned or mandrel forged from solid blanks
Valve and wellhead partsStems, seat rings, bodies, bonnets, blocks and spools
Gears, rolls, wheels and nozzlesNear-net open-die shapes to drawing

Delivery condition can be as-forged with allowance, rough or proof machined, or finish machined to drawing, in condition A or aged to RH950, H950, H1000, H1025, H1050, H1100, H1150 or H1150M.

09

Plant and working envelope

Jiangyin Jiangnan Metal Co., Ltd. has melted and forged on one site in Zhouzhuang Town, Jiangyin City since 1997. 460 people work here, among them 9 senior engineers, 32 intermediate engineers and 140 technicians. The works holds CCS, BV, DNV, LR and NK approvals.

Capacity relevant to this grade
StepEquipmentLimit
Melting25 t electric arc furnace, 25 t and 50 t ladle furnaces, 30 t and 60 t vacuum oxygen decarburisation60 t maximum heat
Remelting3 t and 6 t protective-atmosphere electroslag furnaces, 6 t vacuum arc remelting, 3 t vacuum induction meltingDouble-melt routes without subcontracting
ForgingHydraulic open-die presses at 6,300 t, 4,000 t and 2,000 t; hammers from 750 kg to 5 t30 t heaviest single piece
Ring rollingRadial-axial mills at 6 m, 3 m and 1 mOD 50 mm to 6,000 mm
Heat treatment14 furnaces, including car-bottom to 8,000 × 2,000 × 2,000 mm and two 15 m well-type furnacesVertical quench for long shafts
MachiningVertical lathes to 5,000 mm swing, horizontal lathes to 14 m between centres, CNC deep-hole drilling to 1,600 × 10,000 mmFinish machining in house

Those are plant limits, not grade limits. A precipitation-hardening stainless ring of 6,000 mm is not a normal order; the envelope for 1.4534 is set case by case by the ingot size available from the remelting route and by the solution-treatment quench. Send the size and it will be confirmed before the price goes out.

10

Where the grade is used

Subsea and wellhead

Deepwater production components, wellhead and Christmas-tree parts, valve stems and seat rings for ball, gate, globe, check and plug valves, where cracking resistance matters as much as strength.

Aerospace

Landing-gear parts, structural sections, pins and shafts, normally ordered to AMS 5629 rather than to the EN number.

Rotating equipment

Turbine and compressor rings and shafts, gearbox parts, power-transmission spindles, air compressors and generator components.

Chemical and petrochemical

Chemical and plunger pump shafts and rings, pressure-vessel and heat-exchanger flanges, tube sheets and forged pipe, column and tower internals.

Nuclear

Components needing resistance to stress-corrosion cracking together with high proof strength.

Heavy machinery

Mill and mixer parts, crystalliser equipment, forged rolls and wheels for shipbuilding, pulp and paper and pharmaceutical plant.

11

Testing and certification

Each forging is released against a documented route: melt analysis, forging and reduction record, heat-treatment chart, mechanical tests on a representative piece, non-destructive examination, dimensional report, certificate.

Test methods applied to this grade
TestEquipmentStandard
Chemical analysisSPECTROTEST TXC25 optical emission spectrometerASTM E415
Carbon and sulphurHIR-9440D infrared analyserASTM E1019
Alloy verificationX-Mwt3000TX handheld analyserPositive material identification
TensileWE-600B 600 kN, WDW-300 electronicASTM A370, ISO 6892
ImpactJBN-300 pendulum with DWC-60 bathASTM A370, to minus 60 °C
HardnessTH140 Leeb testerASTM A956, converted per ASTM E140
UltrasonicPXUT-3300, USM35XS, CTS-22ASTM A388, EN 10228-3, SEP 1921
Magnetic particleCYE-3A crack detectorASTM E709
Grain size and structureXJP-6A microscope with mounting and polishing lineASTM E112

EN 10204 3.1 mill certificates are issued as standard. EN 10204 3.2 certificates witnessed by BV, DNV, LR, SGS, TUV or your own inspector are available on request, and should be stated at enquiry stage so the inspection is scheduled rather than added later. Intergranular corrosion testing to ASTM A262 or G28, pitting tests to ASTM G48 and impact testing below minus 60 degrees are placed with an accredited laboratory, with the report issued alongside the mill certificate.

12

Questions buyers ask

What is X3CrNiMoAl13-8-2?

A martensitic precipitation-hardening stainless steel, EN material number 1.4534, containing 12.25 to 13.25 per cent chromium, 7.5 to 8.5 per cent nickel, 2.0 to 2.5 per cent molybdenum and 0.90 to 1.35 per cent aluminium. It is the European designation of UNS S13800, sold as PH 13-8 Mo and covered by ASTM grade XM-13 and AMS 5629. It is specified where high strength has to come with good transverse toughness and resistance to stress-corrosion cracking.

Is it the same as PH 13-8 Mo and UNS S13800?

Yes, the same alloy under different names. The EN specification is tighter on two elements: manganese 0.10 per cent maximum against 0.20, and aluminium 0.90 to 1.20 per cent against 0.90 to 1.35. If your order must meet EN 1.4534 rather than XM-13, say so on the enquiry and the melt is aimed at the narrower range.

Does H900 apply to this grade?

No. H900 is a condition of 17-4 PH. The lowest standard ageing temperature for X3CrNiMoAl13-8-2 is 510 degrees Celsius, which gives H950 and RH950. The standard conditions are A, RH950, H950, H1000, H1025, H1050, H1100, H1150 and H1150M. Drawings that call for 13-8 Mo in H900 usually carry over a note written for 17-4 PH, and the condition has to be agreed before the order is placed.

How does it compare with 17-4 PH?

Both harden by precipitation, but 1.4534 is held to much lower sulphur and phosphorus and is normally double melted, so it carries better toughness across the grain and better resistance to stress-corrosion cracking, particularly in heavy sections. It also reaches higher strength, 1515 MPa minimum in H950 against 17-4 PH. The trade is cost and machinability: it cuts roughly 20 to 30 per cent slower than 17-4 PH in condition A. Where the section is thin and the loading is longitudinal, 17-4 PH is often the cheaper answer.

Which condition should be specified?

H950 or RH950 for maximum strength and hardness. H1000 or H1025 for near-peak strength with better toughness, and for service where stress-corrosion cracking governs, since ageing at 538 degrees or above is the usual recommendation. H1050 to H1100 for a working balance. H1150 or H1150M where toughness and machinability lead. If the part needs heavy machining, order condition A or H1150M and age afterwards, remembering that H1150 and H1150M material must be re-solution treated before it will age again.

Can it be welded?

Yes, by inert-gas shielded and resistance processes, normally in the solution-annealed condition with 13-8 Mo filler, and preheat is not usually needed. Where full weld strength is not required, E308L or ER308L consumables can be used. Solution treating the welded part before ageing gives the best balance of strength, ductility and corrosion resistance, and material welded in an overaged condition must be re-solution treated before it will respond to ageing.

What sizes and weights can be forged in this grade?

The plant rolls rings to 6,000 mm outside diameter and forges single pieces to 30 tonnes, but for a precipitation-hardening stainless the practical limit comes from the remelted ingot and from quenching the section uniformly. Send the outside diameter, bore, height and finished weight, or the drawing, and the size will be confirmed with the quotation. Minimum order is 10 kg with no minimum piece count.

What is needed for a firm price?

Six things: the grade and specification, for example X3CrNiMoAl13-8-2 to ASTM A564 XM-13; dimensions or a drawing in PDF, DWG, DXF or STEP; quantity and expected repeat volume; delivery condition, as-forged, proof machined or finish machined; heat treatment, testing and NDT acceptance class; and the certificate type with destination port. With those in the first email a price normally comes back within two working days.

How long does an order take?

20 to 60 days from order confirmation. This grade sits at the longer end, because the low sulphur and phosphorus limits call for a remelting step, and the solution treatment and ageing add furnace time. Witnessed inspection to EN 10204 3.2, or corrosion testing placed outside, also needs scheduling, so flag both at enquiry stage and they are built into the quoted date.

Quote a X3CrNiMoAl13-8-2 forging

Send a drawing or the dimensions and the condition you need. An English-speaking engineer answers enquiries, and the price comes back with the inspection plan attached rather than as a bare figure.

Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone, WhatsApp and WeChat: +86 189 2135 9659
Email: sales@steelforgepieces.com
Hours: Monday to Saturday, 08:00 to 17:30 China Standard Time, UTC+8

Compiled by the engineering office of Jiangyin Jiangnan Metal Co., Ltd., an integrated melting works and open-die forging factory in Jiangyin, Jiangsu, China, operating since 1997. Figures are drawn from the published requirements for UNS S13800 and 1.4534 under ASTM A564, ASTM A693 and AMS 5629, together with producer data for PH 13-8 Mo. They are given for selection purposes; the properties that apply to an order are those recorded on its mill certificate. Reviewed .