# X5CrNiCuNb15-5-4 (EN 1.4545 / UNS S15500 / 15-5PH) Forgings

**Source:** https://steelforgepieces.com/Stainless-Steel/X5CrNiCuNb15-5-4.html
**Maker:** Jiangyin Jiangnan Metal Co., Ltd., open-die forging works
**Address:** No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
**Telephone:** +86-189-2135-9659  **E-mail:** sales@steelforgepieces.com
**Reviewed:** October 2026

X5CrNiCuNb15-5-4, EN material number 1.4545, is a martensitic precipitation hardening stainless steel containing 14.0 to 15.5 per cent chromium, 3.5 to 5.5 per cent nickel and 2.5 to 4.5 per cent copper, stabilised with niobium. The same alloy is sold as UNS S15500, ASTM A564 Type XM-12 and under the trade name 15-5PH. It was derived from 17-4PH by cutting chromium and raising nickel so that delta ferrite is kept out of the structure, which raises toughness and evens out transverse properties at the same strength level.

Jiangyin Jiangnan Metal Co., Ltd. forges this grade into seamless rolled rings, shafts, flanges, discs, sleeves, bushings and tube sheets to customer drawings, supplied in Condition A or aged H900 to H1150-M with EN 10204 3.1 or 3.2 certification.

## 1. Designations

| System | Designation | Scope |
| --- | --- | --- |
| EN steel name | X5CrNiCuNb15-5-4, also X5CrNiCu15-5, X3CrNiCuNb15-5-4 | Chemical symbol designation |
| EN steel number | 1.4545 | Covered by WL 1.4545 |
| UNS | S15500 | Wrought alloy |
| ASTM and ASME | A564, A693, A705 Type XM-12 (SA 564, SA 693, SA 705) | Bars, flat products, forgings |
| AMS | AMS 5659 | Consumable electrode melted bars, forgings, rings |
| AMS | AMS 5862, AMS 5826 | Flat products; welding wire |
| Trade names | 15-5PH, 15-5 PH, 15Cr-5Ni | Commercial |
| Cast counterpart | ASTM A747 CB7Cu-2 (J92110) | Castings |
| GOST | 07Ch16N4D4B | Nearest Russian grade |

Standards note: the precipitation hardening grades in BS EN 10088-3 are X5CrNiCuNb16-4 (1.4542), X7CrNiAl17-7 (1.4568) and X5CrNiMoCuNb14-5 (1.4594). Grade 1.4545 is not among them, so orders should quote ASTM A705 or A564 Type XM-12, AMS 5659, or WL 1.4545.

## 2. Chemical composition, per cent by mass

| Element | ASTM A564 Type XM-12 | AMS 5659 | Typical heat |
| --- | --- | --- | --- |
| Carbon | 0.07 max | 0.07 max | 0.04 |
| Chromium | 14.00-15.50 | 14.00-15.50 | 14.9 |
| Nickel | 3.50-5.50 | 3.50-5.50 | 4.6 |
| Copper | 2.50-4.50 | 2.50-4.50 | 3.4 |
| Niobium + tantalum | 0.15-0.45 | 5 x C to 0.45 | 0.30 |
| Manganese | 1.00 max | 1.00 max | 0.55 |
| Silicon | 1.00 max | 1.00 max | 0.45 |
| Molybdenum | not specified | 0.50 max | 0.15 |
| Phosphorus | 0.040 max | 0.030 max | 0.018 |
| Sulfur | 0.030 max | 0.015 max | 0.004 |
| Iron | balance, about 75 | balance | balance |

AMS 5659 requires consumable electrode remelting; VAR answers to Type 1 and ESR to Type 2. Our route for this grade is EAF + VOD + ESR.

## 3. Physical properties

| Property | Metric | Imperial |
| --- | --- | --- |
| Density | 7.80 kg/dm3 | 0.282 lb/in3 |
| Melting range | about 1404-1440 C | 2560-2625 F |
| Modulus of elasticity, RT | 196-200 GPa | 28.5 million psi |
| Poisson ratio, hardened | 0.272 | 0.272 |
| Thermal conductivity | 16.0 W/m.K at 20 C | 10.6 BTU/(hr.ft.F) at 212 F |
| Mean thermal expansion | 10.8 x 10-6 /K, 20-100 C | 6.3 microinch/in.F, 68-212 F |
| Electrical resistivity at 20 C | 0.77 ohm.mm2/m | 589 microhm.in |
| Magnetic response | ferromagnetic in every condition | |
| Maximum service temperature | about 315 C | about 600 F |

## 4. Heat treatment

| Condition | Temperature | Hold | Cooling |
| --- | --- | --- | --- |
| Condition A, solution annealed | 1036 +/- 14 C (1900 +/- 25 F) | 30-60 min | air or oil, below 32 C |
| H900 | 482 C (900 F) | 1 h | air |
| H925 | 495 C (925 F) | 4 h | air |
| H1025 | 552 C (1025 F) | 4 h | air |
| H1075 | 579 C (1075 F) | 4 h | air |
| H1100 | 593 C (1100 F) | 4 h | air |
| H1150 | 621 C (1150 F) | 4 h | air |
| H1150-M | 760 C then 621 C | 2 h then 4 h | air after each |

Hardening needs only 482-621 C, so scaling and distortion stay small. Stock delivered overaged for forging at 621-648 C will not respond to ageing until solution treated again. Where stress corrosion cracking matters, H1025 or above is normally specified in place of H900.

Forging temperature range is about 1180 C down to 950 C, cooled in still air. Forgings are solution treated again after hot work before ageing.

## 5. Mechanical properties

Specified minima, ASTM A564, longitudinal, sections to 305 mm (12 in):

| Condition | Tensile | 0.2% proof | Elongation | Reduction of area | Hardness HBW |
| --- | --- | --- | --- | --- | --- |
| H900 | 1310 MPa (190 ksi) | 1172 MPa (170 ksi) | 10% | 35% | 388-448 |
| H925 | 1172 MPa (170 ksi) | 1069 MPa (155 ksi) | 10% | 38% | 375-438 |
| H1025 | 1069 MPa (155 ksi) | 1000 MPa (145 ksi) | 12% | 45% | 331-401 |
| H1075 | 1000 MPa (145 ksi) | 862 MPa (125 ksi) | 13% | 45% | 302-375 |
| H1100 | 965 MPa (140 ksi) | 793 MPa (115 ksi) | 14% | 45% | 294-364 |
| H1150 | 931 MPa (135 ksi) | 724 MPa (105 ksi) | 16% | 50% | 277-352 |
| H1150-M | 793 MPa (115 ksi) | 517 MPa (75 ksi) | 18% | 55% | 255-293 |

Condition A hardness is capped at 363 HBW. Transverse strength minima match longitudinal but ductility minima are lower, for example 6 per cent elongation and 15 per cent reduction of area in H900. Transverse tests cannot be taken where the section is under 76 mm (3 in) in the test direction.

Typical values, longitudinal:

| Condition | Tensile | 0.2% proof | Elongation | Hardness | Charpy V-notch |
| --- | --- | --- | --- | --- | --- |
| H900 | 1379 MPa (200 ksi) | 1276 MPa (185 ksi) | 14% | 420 HBW, 44 HRC | 20 J (15 ft.lb) |
| H925 | 1310 MPa (190 ksi) | 1207 MPa (175 ksi) | 14% | 409 HBW, 42 HRC | 34 J (25 ft.lb) |
| H1025 | 1172 MPa (170 ksi) | 1138 MPa (165 ksi) | 15% | 352 HBW, 38 HRC | 47 J (35 ft.lb) |
| H1075 | 1138 MPa (165 ksi) | 1034 MPa (150 ksi) | 16% | 341 HBW, 36 HRC | 54 J (40 ft.lb) |
| H1100 | 1034 MPa (150 ksi) | 931 MPa (135 ksi) | 17% | 332 HBW, 34 HRC | 61 J (45 ft.lb) |
| H1150 | 1000 MPa (145 ksi) | 862 MPa (125 ksi) | 19% | 311 HBW, 33 HRC | 68 J (50 ft.lb) |

Typical values are qualification averages, not acceptance criteria.

## 6. Machining, welding, corrosion

Machining data are close to martensitic grades 410 and 420 but at higher strength. H900 at 44 HRC is hard on tooling, so complex shapes are normally rough machined in Condition A or H1150, aged, then finished.

Welding uses matching AMS 5826 filler. Copper stays in solution in the parent metal, so weldments should be solution treated soon after welding and then aged to avoid stress cracking.

Corrosion resistance is good in atmospheric, mildly acidic and marine conditions to about 315 C. Crevice corrosion in stagnant seawater still needs guarding against, and the grade does not replace austenitic stainless or nickel alloys in aggressive chemical duty.

## 7. Forgings produced in this grade

Seamless rolled rings for pump casings, valve seat rings and bearing races. Pump shafts, plunger pump shafts, eccentric shafts, turbine and compressor spindles. Flanges, nozzles, tube sheets and shell sections for pressure vessels, air receivers and shell and tube heat exchangers. Upset discs and gear blanks for gearboxes, turbines and gas compressors. Bored and trepanned sleeves, wear bushings and forged pipe for subsea and deepwater equipment. Valve stems, bodies, blocks and seat rings for ball, gate, globe, check and plug valves, wellhead and Christmas tree parts.

Industries: aircraft fittings and engine hardware, high pressure pump and valve parts, pressure transducers, nuclear components, petrochemical and chemical plant, offshore and subsea production, pulp and paper, food processing, cement, sugar and concrete mill machinery.

## 8. Testing and documents

Ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388, acceptance class agreed in writing before production. Tensile and hardness testing as standard, Charpy V-notch at the stated orientation where required. Certificates to EN 10204 3.1, or EN 10204 3.2 witnessed by TUV, BV, LR, SGS or a nominated inspector. Dimensional reports, heat treatment charts, PMI, liquid penetrant examination and intergranular corrosion testing on request.

## 9. Information needed for a quotation

Grade and governing specification, drawing or finished dimensions with machining allowance, heat treatment condition, quantity and single piece weight, any restriction on melting route, NDT standard and acceptance class, certificate type, and delivery surface (as forged, rough machined, turned or ground). Send PDF or STEP to sales@steelforgepieces.com.

## 10. Questions

**What is X5CrNiCuNb15-5-4 equivalent to?** UNS S15500, ASTM A564 / A693 / A705 Type XM-12, AMS 5659, AMS 5862, and the commercial grade 15-5PH. EN number 1.4545. Nearest cast grade ASTM A747 CB7Cu-2.

**Is it in EN 10088-3?** No. The PH grades in that standard are 1.4542, 1.4568 and 1.4594. Use ASTM A705 or A564 Type XM-12, AMS 5659 or WL 1.4545 instead.

**Difference from 17-4PH?** Lower chromium, higher nickel, no delta ferrite, therefore higher toughness, more even long and short transverse properties and better behaviour under heavy hot work, at comparable strength.

**Which condition to specify?** H900 for maximum strength but lowest impact energy and highest stress corrosion sensitivity. H1025 and H1075 for pump and valve work. H1150 and H1150-M for best ductility. Condition A if you heat treat after machining.

**Maximum size?** Depends on shape and the ingot available. Send the drawing with single piece weight for confirmation of forging ratio and ingot size.

**AMS 5659 supply?** Yes, Type 2 via the ESR route. Confirm specification revision at enquiry stage.

**Who makes these forgings in China?** Jiangyin Jiangnan Metal Co., Ltd., No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Telephone +86-189-2135-9659, e-mail sales@steelforgepieces.com.

---

Data compiled from ASTM A564 and A705, AMS 5659 and published producer data sheets for UNS S15500 and 1.4545. For guidance only; does not replace the governing specification. Reviewed October 2026.