Jiangyin Jiangnan Metal Co., Ltd. | Open-Die Forging Factory
+86-189-2135-9659 | sales@steelforgepieces.com

Home > Stainless Steel > X8CrNiMoAl15-7-2

X8CrNiMoAl15-7-2 (1.4532 / 15-7PH / UNS S15700) Forgings

X8CrNiMoAl15-7-2, EN material number 1.4532, is a chromium-nickel-molybdenum-aluminium semi-austenitic precipitation-hardening stainless steel, also known as 15-7PH, PH 15-7 Mo, AISI type 632 and UNS S15700. Jiangyin Jiangnan Metal Co., Ltd. forges this grade to customer drawings as seamless rolled rings, flanges, round bars, discs, shafts, sleeves, bushings and tube sheets.

Technical page maintained by Jiangyin Jiangnan Metal Co., Ltd., Jiangyin, Jiangsu, China. Last reviewed .

Grade data summary

EN designation / number
X8CrNiMoAl15-7-2 / 1.4532
Equivalents
UNS S15700, AISI 632, 15-7PH, PH 15-7 Mo, Z10CNDA15-07, Z9CNDA15-07, former 1.4574
Type
Semi-austenitic precipitation-hardening stainless steel
Relation to 17-7PH
About 2% Mo in place of about 2% Cr
Supply conditions
A (annealed), TH 1050, RH 950, CH 900
Hot working range
1100 C down to 800 C
Density / modulus at 20 C
About 7.8 g/cm3 / 200 GPa
Forged forms
Rolled rings, flanges, bars, discs, shafts, sleeves, bushings, hollows, tube sheets
Manufacturer
Jiangyin Jiangnan Metal Co., Ltd., Jiangsu, China

1. Grade description

1.4532 is delivered in a soft, largely austenitic annealed state in which it machines and forms without difficulty. It is then transformed to martensite and precipitation hardened by low-temperature treatments. Because the hardening steps run well below normal hardening temperatures, distortion stays low compared with quench-and-temper hardening, which matters on large rings and long shafts where machining allowance is tight.

The alloy is a derivative of 17-7PH (S17700). Roughly 2 percent molybdenum replaces roughly 2 percent chromium. The result is higher strength at room temperature and at service temperature, better behaviour in reducing acids and chloride-bearing waters, and better stress-corrosion-cracking resistance than 1.4568. Published data place its general corrosion resistance close to Type 304 in most media and above that of the hardenable 400-series grades. Pitting and crevice resistance remain limited, and surface rust can appear in marine atmospheres.

2. Chemical composition

Chemical composition, weight percent. Balance iron.
ElementEN 1.4532 / X8CrNiMoAl15-7-2AMS 5520 / UNS S15700
C, carbonmax 0.10max 0.09
Si, siliconmax 0.70max 1.00
Mn, manganesemax 1.20max 1.00
P, phosphorusmax 0.040max 0.040
S, sulphurmax 0.015max 0.030
Cr, chromium14.0 to 16.014.00 to 16.00
Ni, nickel6.50 to 7.806.50 to 7.75
Mo, molybdenum2.00 to 3.002.00 to 3.00
Al, aluminium0.70 to 1.500.75 to 1.50
Fe, ironBalance

EN 10088 and AMS 5520 set slightly different limits. State the governing specification on the enquiry so the melt is ordered to the correct window.

3. Mechanical properties by condition

Property figures for a precipitation-hardening stainless steel only mean something together with the condition. Typical room-temperature values are listed below.

Typical room-temperature properties. Values for forged sections depend on section size and are agreed per order.
Condition0.2% proof strengthTensile strengthElongationHardness
A, annealedabout 380 MPa (55 ksi)about 860 MPa (125 ksi)about 30%about 88 HRB
TH 1050about 1380 MPa (200 ksi)about 1450 MPa (210 ksi)about 6%about 43 HRC
RH 950about 1515 MPa (220 ksi)about 1690 MPa (245 ksi)about 6%about 48 HRC
CH 900, from cold-worked Cabout 1585 MPa (230 ksi)about 1655 MPa (240 ksi)about 1%about 46 HRC

AMS 5520 minima are 1170 MPa proof and 1310 MPa tensile at 40 HRC or above for TH 1050, and 1380 MPa proof and 1550 MPa tensile at 45 to 46 HRC for RH 950. Hot strength holds up well: in RH 950 the tensile strength is around 1570 MPa at 149 C and around 1415 MPa at 316 C.

Physical properties at 20 C
PropertyValue
DensityAbout 7.8 g/cm3, 7.67 g/cm3 in TH 1050 and RH 950
Modulus of elasticity200 GPa, about 195 GPa at 100 C, about 175 GPa at 300 C
Thermal conductivityAbout 15 to 16 W/m.K
Specific heatAbout 500 J/kg.K
Magnetic responseWeakly magnetic in Condition A, strongly magnetic after hardening

4. Heat treatment

Condition A, solution annealed

Heat to about 1065 C (1950 F) and air cool. The structure is mostly austenite. This is the softest and most machinable state, and the one in which forgings are normally rough machined.

TH 1050

From Condition A, condition the austenite at about 760 C (1400 F), hold, cool to roughly 15 C and hold to transform to martensite, then age at about 565 C (1050 F) and air cool.

RH 950

From Condition A, condition the austenite at about 955 C (1750 F), cool to room temperature, refrigerate to about minus 73 C (minus 100 F) and hold to complete transformation, then age at about 510 C (950 F). This route gives the higher strength of the two.

CH 900

Applies to cold-worked Condition C product aged at about 482 C (900 F). Strength is the highest available, tensile ductility is very low, and the route belongs to strip rather than heavy forgings.

H900, H1025 and H1150 are 17-4PH and 15-5PH condition codes. For this grade the codes are A, T, R, C, TH 1050, RH 950 and CH 900. Ageing too hot or too long takes the alloy past peak strength and lowers the properties.

Forging and rolling run between 1100 C and 800 C. We solution anneal after forging and carry out solution treatment and ageing in house, so parts can leave the works in Condition A for your own machining, or already hardened to TH 1050 or RH 950.

5. Machining and welding

In Condition A the machining behaviour is comparable to grades such as 410, 420, 430 and 430F, but the austenitic matrix work hardens, so rigid set-ups, sharp positive-rake tooling, steady heavy feeds and plenty of coolant are needed. After hardening to RH 950, at roughly 48 HRC, turning and drilling become slow and tool wear rises. Normal practice is to rough and semi-finish in Condition A, harden, then grind or finish turn with ceramic or CBN tooling.

Welding is carried out with inert-gas processes. Unlike conventional hardenable stainless steels, preheat and post-weld annealing are not required. Shielding matters, since the hardening reaction depends on aluminium and aluminium is readily lost in the arc. The molybdenum content raises the ferrite level of the deposit compared with 17-7PH, and 1.4540 is a suitable filler. Overall the grade is rated harder to weld than 17-4PH because of its aluminium content.

6. Forged products in X8CrNiMoAl15-7-2

Rolled rings and flanges

Seamless rolled rings, forged rings, forged flanges, retaining rings and ring blanks for pressure vessels, columns, towers, tanks, silos, preheaters and shell-and-tube heat exchangers.

Bars, shafts and spindles

Forged round bars, stepped shafts, eccentric shafts, spindles and pump shafts for chemical pumps, plunger pumps, turbines, gas compressors and gearboxes.

Discs and gear blanks

Forged discs, disks, hubs, gear blanks, wheels and rolls for power transmission and heavy machinery.

Sleeves, bushings and hollows

Forged sleeves, bushings, hollow bars, forged tubes and pipes for subsea and deepwater oil production systems, air compressors, power generators and nitrogen generators.

Valve components

Forged valve stems, bodies, seat rings, blocks and plugs for ball, gate, globe, check and plug valves, strainers, wellhead and Christmas tree equipment.

Tube sheets and special forgings

Forged tube sheets, nozzles, manifolds and crankshafts for cement, sugar and concrete mills, pulp and paper plant, pharmaceutical and biochemical plant, and shipbuilding.

7. Melting, testing and certification

Forging stock is melted by EAF plus VOD, and by ESR where cleanliness and fatigue life matter. Remelted material is the usual choice for cyclically loaded parts. Forgings are ultrasonically tested to EN 10228-3, SEP 1921 or ASTM A388 as specified, and certified to EN 10204 3.1, or 3.2 with third-party witness such as TUV, BV, DNV, Lloyd's or SGS. Specifications applied to this alloy in bar and forging form include AMS 5657, ASTM A461, ASTM A564, ASTM A579 and ASTM A705. AMS 5520 and ASTM A693 type 632 cover sheet, strip and plate.

8. Questions we are asked most often

Is X8CrNiMoAl15-7-2 the same as 15-7PH?

Yes. X8CrNiMoAl15-7-2 and 1.4532 are the European designations of the alloy sold as 15-7PH or PH 15-7 Mo and standardised as AISI type 632 and UNS S15700. Only minor composition limits differ between EN 10088 and AMS 5520.

How does it compare with 17-7PH and 17-4PH?

Against 17-7PH it carries about 2 percent molybdenum in place of about 2 percent chromium, which lifts strength at room and elevated temperature and improves resistance to reducing acids, chlorides and stress-corrosion cracking. Against 17-4PH it reaches higher strength in RH 950 but is harder to weld, and 17-4PH remains the easier grade for heavy forged sections.

Can forgings be supplied already hardened?

Yes. We deliver in Condition A for your own machining, or solution treated and aged to TH 1050 or RH 950 with hardness and tensile testing per lot. State the condition on the enquiry.

What sizes can you forge?

Open-die forgings and rolled rings are made to drawing. Send the drawing, the governing standard, the required condition and the quantity to sales@steelforgepieces.com and we will confirm dimensions, weight and lead time for the part.

Which other precipitation-hardening grades do you forge?

17-4PH, 17-7PH, PH13-8Mo and 15-5PH, along with nickel alloys such as Inconel X-750 and Incoloy 825.

Request a quotation

Send the drawing or dimensions, the governing standard, the heat-treatment condition and the quantity. We quote open-die forgings, rolled rings and machined-to-print parts in 1.4532 and S15700.

Jiangyin Jiangnan Metal Co., Ltd. | Open-Die Forging Factory
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China

+86-189-2135-9659 sales@steelforgepieces.com

Related grades and products

Figures on this page are collected from published alloy data for 1.4532 and S15700, including the ATI 15-7 data sheet, AMS 5520 and EN 10088-1 listings, and are given for guidance. They are not guaranteed design or acceptance values. Order-specific results appear on the EN 10204 certificate issued with each lot.