# X8CrNiSiN21-11 Forgings (EN 1.4835 / 253MA / UNS S30815)

Supplier: Jiangyin Jiangnan Metal Co., Ltd., Open-Die Forging Factory
Address: No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel: +86-189-2135-9659
Email: sales@steelforgepieces.com
Page: https://steelforgepieces.com/Stainless-Steel/X8CrNiSiN21-11.html
Last reviewed: 11 October 2026

Designations: X9CrNiSiNCe21-11-2 | 1.4835 | 253MA | UNS S30815 | SS 2368 | ISO X7CrNiSiNCe21-11 | 1.4893

## Summary

X8CrNiSiN21-11 is a designation listed for the heat-resisting austenitic stainless steel X9CrNiSiNCe21-11-2, EN material number 1.4835, sold commercially as 253MA and in the United States as UNS S30815. It is a 21 % chromium, 11 % nickel austenitic steel micro-alloyed with silicon, cerium and nitrogen, intended for service above 550 °C, with an optimum structural range of 850 to 1100 °C and oxidation resistance in air reported up to 1150 °C.

Jiangyin Jiangnan Metal Co., Ltd. forges this grade into rings, seamless rolled rings, flanges, bars, discs, sleeves, shafts and tube sheets, supplied with ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388 and EN 10204 3.1 or 3.2 certification. Pricing is quoted per drawing.

## Chemical composition, % by mass, balance Fe

| Designation | C | Si | Mn | P | S | Cr | Ni | Ce | N |
|---|---|---|---|---|---|---|---|---|---|
| X8CrNiSiN21-11 / X7CrNiSiNCe21-11 / S30815 | 0.05-0.10 | 1.40-2.00 | ≤0.80 | ≤0.040 | ≤0.030 | 20.00-22.00 | 10.00-12.00 | 0.030-0.080 | 0.14-0.20 |
| EN 1.4835, X9CrNiSiNCe21-11-2 (EN 10095) | 0.05-0.12 | 1.40-2.50 | ≤1.00 | ≤0.045 | ≤0.015 | 20.00-22.00 | 10.00-12.00 | 0.030-0.080 | 0.12-0.20 |

Sulphur can be restricted to 0.010 % maximum and any element tightened on request.

The raised silicon content together with the cerium addition stabilises the protective chromium oxide layer, which is the mechanism behind the oxidation resistance. Nitrogen raises strength at temperature and reduces loss of toughness from sigma phase formation. Together these additions allow 1.4835 to be used in thinner sections than conventional chromium nickel silicon heat-resisting steels.

## Mechanical and physical properties, solution annealed (+AT)

| Property | Symbol | Value |
|---|---|---|
| Tensile strength | Rm | 650-850 MPa |
| Yield point | Re | 310 MPa |
| Elongation | A | above 37 % |
| Hardness | HB | below 210 HB |
| Density | rho | 7.80 kg/dm3 |
| Specific heat capacity, 20-100 °C | cp | 500 J/(kg·K) |
| Coefficient of linear expansion, 20-100 °C | alpha | 17.0-19.5 x10-6 1/K |
| Thermal conductivity at 20 °C | lambda | 15 W/(m·K) |
| Electrical resistivity | rho el | 0.85 x10-4 ohm·cm |
| Magnetic response | - | Non-magnetic annealed, may become slightly magnetic after cold work or welding |

## Creep rupture strength and creep limit, MPa

| Property | 600 °C | 700 °C | 800 °C | 900 °C | 1000 °C |
|---|---|---|---|---|---|
| Creep rupture Rz/1 000h | 238 | 105 | 50 | 24 | 12 |
| Creep rupture Rz/10 000h | 157 | 63 | 27 | 13 | 7 |
| Creep rupture Rz/100 000h | 88 | 35 | 15 | 8 | 4 |
| Creep limit R1/1 000h | 170 | 66 | 31 | 15.5 | 8 |
| Creep limit R1/10 000h | 126 | 45 | 19 | 10 | 5 |
| Creep limit R1/100 000h | 80 | 26 | 11 | 6 | 3 |

## Heat treatment and hot working

| Operation | Temperature | Time | Cooling |
|---|---|---|---|
| Softening, solution annealing | 1020-1120 °C | 5-20 min | Rapid, in air or water |
| Stress relief annealing | 850-950 °C | under 30 min | Fast in air |
| Hot forging, thermo-mechanical working | 900-1150 °C | - | Per forging schedule |
| Hot bending | 850-1100 °C | - | - |

850 to 950 °C is a stress relief treatment only. It does not replace solution annealing at 1020 to 1120 °C, which restores the austenitic structure after hot forging. Components cold bent and destined for service above 800 °C are normally annealed afterwards.

## Forming, welding and machining

Forming: cold formed like other high-alloy austenitic steels; the nitrogen content means higher forming forces than 1.4841; springback is pronounced; ductility is considerably better than ferritic heat-resisting grades.

Welding: SMAW, GTAW, plasma arc and submerged arc. Use low heat input and matching EN 1.4835 filler. TIG and MIG give the best creep performance. Hardenable by cold work only.

Machining: work-hardening grade requiring sharp tooling, rigid setups and positive feed. Low sulphur means no free-machining additives, so reduced speeds apply. Rough or finish machined forgings available to drawing.

Service atmospheres: chromium oxide scale gives oxidation resistance reported to 1150 °C in air; good in carburising and nitriding atmospheres although AISI 310 and 314 perform better; sulphur compound resistance approaches ferritic grades 1.4742 and 1.4762; water vapour can cut maximum service temperature by up to 100 °C.

## Comparison with neighbouring grades

| Comparison | Reported behaviour |
|---|---|
| Against 309 stainless | Rolled Alloys reports oxidation resistance of RA 253 MA good to 2000 °F (1093 °C), superior to 309, with creep strength twice that of 309 and 310 above 1600 °F |
| Against 310 stainless | Oxidation performance comparable to 310; in strongly carburising atmospheres 310 and 314 remain better |
| Against X15CrNiSi25-21 (1.4841) | Lower chromium and nickel content, reducing cost, often allowing smaller sections and thinner walls |
| Against 1.4818 (153 MA, S30415) | A different, leaner 19Cr-10Ni cerium grade; not a direct substitute |

## Applications

Published application lists cover high-temperature plant rather than wet corrosion service: combustion chambers, recuperators and heat exchangers, heat treatment furnace tubes and fixtures, radiant and radiator tubes, air heating tubes in sulphuric acid gas converters, thermocouple tubes, burner components, exhaust manifolds, turbine and fan rotors, impact separators, ash hopper covers, furnace refractory anchors, circulating fluidised bed boiler parts, pipe hooks and tubular guards, glass foundry moulds, styrene reactor and convection tubes, and steelworks, glass and cement industry equipment.

Forged shapes produced for these duties: seamless rolled rings and casing rings, flanges and tube sheets, shafts and spindles, discs and blanks, sleeves and bushings, hollow forged tubes, nozzles, valve bodies, seat rings and stems.

For aqueous or acid corrosion service, a duplex, 6Mo or nickel alloy grade may be the correct material instead.

## Manufacturing and quality control

Melting and forging: EAF and VOD refining, ESR remelting where cleanliness is critical, open-die forging and seamless ring rolling, forging range 900 to 1150 °C with controlled reduction ratio, solution annealing after forging at 1020 to 1120 °C.

Testing and documentation: ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388; chemical analysis, tensile, impact and hardness testing; intergranular corrosion and grain size testing on request; EN 10204 3.1 certificates, or 3.2 with third party witness.

## Frequently asked questions

**Is X8CrNiSiN21-11 the same material as 253MA?**
X8CrNiSiN21-11 appears in published cross reference lists as an alternative designation within the X9CrNiSiNCe21-11-2 / 1.4835 / 253MA / UNS S30815 family, alongside 1.4893, SS 2368 and ISO X7CrNiSiNCe21-11. Such cross references are indicative rather than contractual, so confirm the exact specification on the purchase order.

**What is the maximum service temperature?**
Atlas Steels and AZoM state that 253MA resists oxidation at temperatures up to 1150 °C, with 850 to 1100 °C quoted as the most suitable structural range. Water vapour can lower that ceiling by up to 100 °C.

**Which heat treatment should be specified?**
Solution annealing at 1020 to 1120 °C with rapid cooling in air or water, the +AT condition. Stress relief at 850 to 950 °C is an additional step where residual stress must be reduced, not a substitute.

**What sizes and shapes can be forged?**
Rolled rings, flanges, discs, bars, sleeves, shafts, tube sheets and hollow tubes to customer drawing. Send the drawing or finished dimensions with tolerances, quantity, test requirements and certificate level to sales@steelforgepieces.com.

**Is third party certification available?**
EN 10204 3.1 as standard. EN 10204 3.2 with inspection by TUV, SGS, BV or Lloyd's can be arranged when specified at order stage.

## Request a quotation

Jiangyin Jiangnan Metal Co., Ltd., Open-Die Forging Factory
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel: +86-189-2135-9659
Email: sales@steelforgepieces.com

Include grade and standard, drawing or rough dimensions, quantity, required heat treatment condition, NDT requirements and certificate level.

## Standards and data sources

- EN 10095, Heat Resisting Steels and Nickel Alloys; EN 10088-1, List of Stainless Steels
- Virgamet grade datasheet, X9CrNiSiNCe21-11-2 / 1.4835 / 253MA
- Atlas Steels and AZoM grade data sheets, Stainless Steel 253MA (UNS S30815)
- Rolled Alloys, RA 253 MA versus 309/310
- Fushun Special Steel datasheet, 1.4835 / X9CrNiSiNCe21-11-2

Published property values are indicative. Contractual values are those stated on the material certificate.