X5CrNiCuNb15-5-4 (EN 1.4545 / UNS S15500 / 15-5PH) Forgings
Seamless rolled rings, forged shafts, flanges, discs, sleeves, bushings and tube sheets. ESR melted, supplied in Condition A or aged H900 to H1150-M, certified to EN 10204 3.1 or 3.2.
X5CrNiCuNb15-5-4, EN material number 1.4545, is a martensitic precipitation hardening stainless steel containing 14.0 to 15.5 per cent chromium, 3.5 to 5.5 per cent nickel and 2.5 to 4.5 per cent copper, stabilised with niobium. The same alloy is sold as UNS S15500, ASTM A564 Type XM-12 and under the trade name 15-5PH. It was derived from 17-4PH by cutting chromium and raising nickel so that delta ferrite is kept out of the structure, which raises toughness and evens out transverse properties at the same strength level.
Jiangyin Jiangnan Metal Co., Ltd. forges this grade into rings, shafts, flanges, discs and sleeves to customer drawings at its works in Jiangyin, Jiangsu Province, China. Telephone +86-189-2135-9659, e-mail sales@steelforgepieces.com.
- EN number
- 1.4545
- UNS
- S15500
- ASTM type
- XM-12
- Aerospace spec
- AMS 5659
- Structure
- Martensitic PH
- Service limit
- approx. 315 C (600 F)
1. Designations and Equivalent Grades
This alloy appears under several names depending on which body issued the specification, and mixed designations on an enquiry are a common cause of ordering errors. The following all refer to the same grade.
| System | Designation | Scope |
|---|---|---|
| EN steel name | X5CrNiCuNb15-5-4, also written X5CrNiCu15-5 and X3CrNiCuNb15-5-4 | Chemical symbol designation |
| EN steel number | 1.4545 | Covered by WL 1.4545 |
| UNS | S15500 | Wrought alloy |
| ASTM and ASME | A564, A693, A705 Type XM-12 (SA 564, SA 693, SA 705) | Bars and shapes, flat products, forgings |
| AMS | AMS 5659 | Consumable electrode melted bars, forgings and rings |
| AMS | AMS 5862, AMS 5826 | Sheet, strip and plate; welding wire |
| Trade names | 15-5PH, 15-5 PH, 15Cr-5Ni | Commercial designations |
| Cast counterpart | ASTM A747 Type CB7Cu-2 (J92110) | Castings |
| GOST | 07Ch16N4D4B | Nearest Russian grade |
Standards note. The precipitation hardening grades listed in BS EN 10088-3 are X5CrNiCuNb16-4 (1.4542), X7CrNiAl17-7 (1.4568) and X5CrNiMoCuNb14-5 (1.4594). Grade 1.4545 is not one of them, so an order for X5CrNiCuNb15-5-4 forgings should quote ASTM A705 or A564 Type XM-12, AMS 5659, or WL 1.4545. We confirm the governing specification on the order acknowledgement.
2. Chemical Composition
Limits below follow ASTM A564 and A705 Type XM-12 and AMS 5659. Each heat arrives with a mill analysis and is checked again on our own spectrometer before the ingot goes to the press.
| Element | ASTM A564 Type XM-12 | AMS 5659 | Typical heat |
|---|---|---|---|
| Carbon, C | 0.07 max | 0.07 max | 0.04 |
| Chromium, Cr | 14.00 to 15.50 | 14.00 to 15.50 | 14.9 |
| Nickel, Ni | 3.50 to 5.50 | 3.50 to 5.50 | 4.6 |
| Copper, Cu | 2.50 to 4.50 | 2.50 to 4.50 | 3.4 |
| Niobium plus tantalum | 0.15 to 0.45 | 5 x C to 0.45 | 0.30 |
| Manganese, Mn | 1.00 max | 1.00 max | 0.55 |
| Silicon, Si | 1.00 max | 1.00 max | 0.45 |
| Molybdenum, Mo | not specified | 0.50 max | 0.15 |
| Phosphorus, P | 0.040 max | 0.030 max | 0.018 |
| Sulfur, S | 0.030 max | 0.015 max | 0.004 |
| Iron, Fe | Balance, about 75 per cent | ||
AMS 5659 calls for consumable electrode remelting. Vacuum arc remelted material answers to Type 1 and electroslag remelted material to Type 2. Our normal route for this grade is EAF plus VOD plus ESR.
3. Physical Properties
| Property | Metric | Imperial |
|---|---|---|
| Density | 7.80 kg/dm3 | 0.282 lb/in3 |
| Melting range | about 1404 to 1440 C | 2560 to 2625 F |
| Modulus of elasticity, room temperature | 196 to 200 GPa | 28.5 million psi |
| Poisson ratio, hardened | 0.272 | |
| Thermal conductivity | 16.0 W/m.K at 20 C | 10.6 BTU/(hr.ft.F) at 212 F |
| Mean coefficient of thermal expansion | 10.8 x 10-6 /K, 20 to 100 C | 6.3 microinch/in.F, 68 to 212 F |
| Electrical resistivity at 20 C | 0.77 ohm.mm2/m | 589 microhm.in |
| Magnetic response | Ferromagnetic in every condition | |
At 315 C the modulus falls to roughly 91 per cent of the room temperature figure. The alloy keeps useful strength and corrosion resistance to about that temperature and is not intended for service above it.
4. Heat Treatment
Properties in this grade come almost entirely from the ageing condition, so the condition has to appear on the purchase order. Solution treatment and ageing are done in our own furnaces and the charts go out with the documents.
| Condition | Temperature | Hold | Cooling |
|---|---|---|---|
| Condition A, solution annealed | 1036 +/- 14 C (1900 +/- 25 F) | 30 to 60 min | Air or oil, down below 32 C (90 F) |
| H900 | 482 C (900 F) | 1 h | Air |
| H925 | 495 C (925 F) | 4 h | Air |
| H1025 | 552 C (1025 F) | 4 h | Air |
| H1075 | 579 C (1075 F) | 4 h | Air |
| H1100 | 593 C (1100 F) | 4 h | Air |
| H1150 | 621 C (1150 F) | 4 h | Air |
| H1150-M, double overaged | 760 C (1400 F) then 621 C (1150 F) | 2 h then 4 h | Air after each step |
Hardening needs only 482 to 621 C, so scaling and distortion during ageing stay small. That is the main practical reason this grade is chosen for parts that are machined close to size before heat treatment. Stock delivered overaged for forging at 621 to 648 C will not respond to ageing until it has been solution treated again. Where stress corrosion cracking is a concern, H1025 or a higher ageing temperature is normally specified in place of H900.
5. Mechanical Properties
5.1 Specified minima, ASTM A564, longitudinal, sections to 305 mm (12 in)
| Condition | Tensile strength | 0.2 per cent proof stress | Elongation | Reduction of area | Hardness HBW |
|---|---|---|---|---|---|
| H900 | 1310 MPa (190 ksi) | 1172 MPa (170 ksi) | 10 % | 35 % | 388 to 448 |
| H925 | 1172 MPa (170 ksi) | 1069 MPa (155 ksi) | 10 % | 38 % | 375 to 438 |
| H1025 | 1069 MPa (155 ksi) | 1000 MPa (145 ksi) | 12 % | 45 % | 331 to 401 |
| H1075 | 1000 MPa (145 ksi) | 862 MPa (125 ksi) | 13 % | 45 % | 302 to 375 |
| H1100 | 965 MPa (140 ksi) | 793 MPa (115 ksi) | 14 % | 45 % | 294 to 364 |
| H1150 | 931 MPa (135 ksi) | 724 MPa (105 ksi) | 16 % | 50 % | 277 to 352 |
| H1150-M | 793 MPa (115 ksi) | 517 MPa (75 ksi) | 18 % | 55 % | 255 to 293 |
In Condition A hardness is capped at 363 HBW. Transverse strength minima match the longitudinal figures but the ductility minima are lower, for instance 6 per cent elongation and 15 per cent reduction of area in H900. Transverse tests cannot be taken where the section is under 76 mm (3 in) in the test direction.
5.2 Typical values, longitudinal
| Condition | Tensile strength | 0.2 per cent proof stress | Elongation | Hardness | Charpy V-notch |
|---|---|---|---|---|---|
| H900 | 1379 MPa (200 ksi) | 1276 MPa (185 ksi) | 14 % | 420 HBW, 44 HRC | 20 J (15 ft.lb) |
| H925 | 1310 MPa (190 ksi) | 1207 MPa (175 ksi) | 14 % | 409 HBW, 42 HRC | 34 J (25 ft.lb) |
| H1025 | 1172 MPa (170 ksi) | 1138 MPa (165 ksi) | 15 % | 352 HBW, 38 HRC | 47 J (35 ft.lb) |
| H1075 | 1138 MPa (165 ksi) | 1034 MPa (150 ksi) | 16 % | 341 HBW, 36 HRC | 54 J (40 ft.lb) |
| H1100 | 1034 MPa (150 ksi) | 931 MPa (135 ksi) | 17 % | 332 HBW, 34 HRC | 61 J (45 ft.lb) |
| H1150 | 1000 MPa (145 ksi) | 862 MPa (125 ksi) | 19 % | 311 HBW, 33 HRC | 68 J (50 ft.lb) |
Typical values are averages from qualification testing and are not acceptance criteria. Impact energy in H900 is low. Where a Charpy figure forms part of the design, specify H1025 or above.
6. Forging, Machining and Welding
Forging practice
We forge X5CrNiCuNb15-5-4 between about 1180 C and 950 C and cool in still air. Because the balanced 15Cr 5Ni 4Cu chemistry keeps delta ferrite out, the grade takes heavy upsetting and hot flattening better than 17-4PH, which is why it gets specified for deeply worked rings and large upset discs. After forging the parts go back for solution treatment at 1036 +/- 14 C and are cooled below 32 C before ageing. We do not ship aged parts that have missed the re-solution step after hot work.
Machining
The alloy cuts in Condition A and in the aged conditions, with speeds and feeds close to other martensitic stainless grades such as 410 and 420 but at higher strength. H900 material at 44 HRC is hard on tooling. For complicated shapes we normally rough machine in Condition A or H1150, age, then finish, which keeps both distortion and tool cost down.
Welding
Welding is workable with matching AMS 5826 filler. Copper stays in solution in the parent metal, so a welded assembly should be solution treated soon after welding and then aged, otherwise stress cracking is a risk. Tell us at enquiry stage if the forging is going into a weldment, because that changes the delivery condition we recommend.
Corrosion resistance
Resistance is good in atmospheric, mildly acidic and marine conditions and holds to roughly 315 C (600 F). Crevice corrosion in stagnant seawater still needs guarding against, and the grade does not replace austenitic stainless or nickel alloys in aggressive chemical duty.
7. Forgings We Produce in This Grade
Everything is forged to drawing or to a stated standard. We can quote from a drawing, a dimensioned sketch, or simply an outside diameter, bore and height together with the required condition.
Seamless rolled rings
Radial and axial rolled rings for pump casings, valve seat rings and bearing races, supplied rough machined or with an allowance to your print.
Shafts and spindles
Pump shafts, plunger pump shafts, eccentric shafts, turbine and compressor spindles. Step turning and centreless grinding available.
Flanges and tube sheets
Flanges, nozzles, tube sheets and shell sections for pressure vessels, air receivers and shell and tube heat exchangers.
Discs, blanks and gear blanks
Upset discs and gear blanks for power transmission, gearboxes, turbines and gas compressors.
Sleeves, bushings and hollow bar
Bored and trepanned sleeves, wear bushings and forged pipe sections for subsea and deepwater production equipment and compressors.
Valve components
Valve stems, bodies, blocks and seat rings for ball, gate, globe, check and plug valves, wellhead and Christmas tree parts included.
Industries served
Aircraft fittings and engine hardware, high pressure pump and valve parts, pressure transducers, nuclear components, petrochemical and chemical process plant, offshore and subsea production systems, pulp and paper, food processing plant, and cement, sugar and concrete mill machinery.
8. Testing, Inspection and Documents
Every forging leaves with a document package matched to the order. Ultrasonic testing is carried out to EN 10228-3, SEP 1921 or ASTM A388 as specified, with the acceptance class agreed in writing before production starts. Mechanical testing covers tensile and hardness, plus Charpy V-notch at the stated orientation and location where required. Certificates are issued to EN 10204 3.1, or to EN 10204 3.2 witnessed by a third party such as TUV, BV, LR, SGS or an inspector you nominate. Dimensional reports, heat treatment charts, positive material identification, liquid penetrant examination and intergranular corrosion testing are available on request.
9. What We Need to Quote
Send the grade and governing specification, for example X5CrNiCuNb15-5-4 to ASTM A705 Type XM-12, together with the drawing or the finished dimensions and machining allowance, the heat treatment condition wanted, quantity and single piece weight, any restriction on melting route, the NDT standard and acceptance class, the certificate type, and the delivery surface, whether as forged, rough machined, turned or ground. PDF or STEP files go to sales@steelforgepieces.com and a quotation normally follows within one working day.
10. Questions We Are Often Asked
What is X5CrNiCuNb15-5-4 equivalent to?
UNS S15500, ASTM A564, A693 and A705 Type XM-12, AMS 5659 for bars, forgings and rings, AMS 5862 for flat products, and the commercial grade 15-5PH. The EN material number is 1.4545. The nearest cast grade is ASTM A747 CB7Cu-2.
Is X5CrNiCuNb15-5-4 listed in EN 10088-3?
No. The precipitation hardening grades in that standard are X5CrNiCuNb16-4 (1.4542), X7CrNiAl17-7 (1.4568) and X5CrNiMoCuNb14-5 (1.4594). Use ASTM A705 or A564 Type XM-12, AMS 5659 or WL 1.4545 on the order instead.
Is X5CrNiCuNb15-5-4 better than 17-4PH?
It is a different balance rather than a straight upgrade. Lower chromium and higher nickel remove delta ferrite, which lifts toughness and evens out long and short transverse properties, and it takes heavy hot work more readily. Strength in matching ageing conditions is much the same. For parts loaded through the thickness, and for heavily upset forgings, 15-5PH is usually the sounder choice. For simple bar-machined parts 17-4PH is often picked on cost and availability.
Which condition should I specify?
H900 gives the highest strength and hardness but the lowest impact energy and the greatest sensitivity to stress corrosion cracking. H1025 and H1075 are the usual middle ground for pump and valve parts. H1150 and H1150-M give the best ductility and toughness. If you intend to machine the part yourself, order Condition A and heat treat after machining.
What size can you forge in this grade?
That depends on the shape and on the ingot available for the heat. Send the drawing with the single piece weight and we will confirm feasibility, forging ratio and ingot size before quoting.
Can you supply to AMS 5659?
AMS 5659 requires consumable electrode remelted material, and ESR answers to Type 2. Our standard route for this grade is EAF plus VOD plus ESR, so AMS 5659 Type 2 can be supported. Confirm the specification revision and any customer-specific requirements at enquiry stage so the right heat is reserved.
Who makes these forgings in China?
Jiangyin Jiangnan Metal Co., Ltd., No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Telephone +86-189-2135-9659, e-mail sales@steelforgepieces.com.
Ask for a Price on X5CrNiCuNb15-5-4 Forgings
Send the drawing, the dimensions or the specification. You get back a price, the forging route, the heat treatment plan and a lead time, normally inside one working day.
E-mail sales@steelforgepieces.com Call +86-189-2135-9659
Jiangyin Jiangnan Metal Co., Ltd., No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Related Grades and Forms
Compare with 17-4PH (1.4542 / S17400), 17-7PH (1.4568) and PH13-8Mo, or see this grade as 15-5PH forged rings and forged bars. For hotter or more corrosive duty see our nickel alloy forgings, among them Inconel X-750 and Incoloy 825.
Data on this page are drawn from ASTM A564 and A705, AMS 5659 and published producer data sheets for UNS S15500 and 1.4545. They are given for guidance, do not replace the governing specification and are not a warranty for any particular application. Reviewed October 2026. A plain text version of this page is available at X5CrNiCuNb15-5-4.md.