X8CrNiSiN21-11 is a designation listed for the heat-resisting austenitic stainless steel X9CrNiSiNCe21-11-2, EN material number 1.4835, sold commercially as 253MA and in the United States as UNS S30815. It is a 21 % chromium, 11 % nickel austenitic steel micro-alloyed with silicon, cerium and nitrogen, intended for service above 550 °C, with an optimum structural range of 850 to 1100 °C and oxidation resistance in air reported up to 1150 °C.

Jiangyin Jiangnan Metal Co., Ltd., an open-die forging factory at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, forges this grade into rings, seamless rolled rings, flanges, bars, discs, sleeves, shafts and tube sheets, supplied with ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388 and EN 10204 3.1 or 3.2 certification. Tel +86-189-2135-9659, email sales@steelforgepieces.com.

Chemical Composition

The table below sets the classic X8CrNiSiN21-11 / ISO X7CrNiSiNCe21-11 analysis against the wider EN 1.4835 limits of EN 10095. Both describe the same cerium and nitrogen bearing 21Cr-11Ni austenitic family. Heats we melt are normally aimed at the narrower window.

Chemical composition, % by mass, balance Fe
DesignationCSiMn PSCrNi CeN
X8CrNiSiN21-11 / X7CrNiSiNCe21-11 / S30815 0.05-0.101.40-2.00≤0.80≤0.040≤0.030 20.00-22.0010.00-12.000.030-0.0800.14-0.20
EN 1.4835, X9CrNiSiNCe21-11-2 (EN 10095) 0.05-0.121.40-2.50≤1.00≤0.045≤0.015 20.00-22.0010.00-12.000.030-0.0800.12-0.20

Sulphur can be restricted to 0.010 % maximum and any element tightened on request. State the target analysis on the enquiry and it is written into the heat specification.

Function of the cerium and nitrogen additions

The raised silicon content together with the rare earth cerium addition stabilises the protective chromium oxide surface layer, and this is the mechanism behind the oxidation resistance of the grade. The nitrogen addition raises strength at temperature and reduces loss of toughness from sigma phase formation. Together these additions allow 1.4835 to be used in thinner sections than conventional chromium nickel silicon heat-resisting steels.

Mechanical and Physical Properties

Solution annealed condition (+AT), published datasheet values to EN 10095
PropertySymbolValue
Tensile strengthRm650-850 MPa
Yield pointRe310 MPa
ElongationAabove 37 %
HardnessHBbelow 210 HB
Densityρ7.80 kg/dm³
Specific heat capacity, 20-100 °Ccp500 J/(kg·K)
Coefficient of linear expansion, 20-100 °Cα17.0-19.5 ×10-6 1/K
Thermal conductivity at 20 °Cλ15 W/(m·K)
Electrical resistivityρel0.85 ×10-4 Ω·cm
Magnetic response-Non-magnetic when annealed, may become slightly magnetic after cold work or welding

Values given for information. Acceptance values for a specific forging are agreed at order stage and reported on the EN 10204 certificate.

Creep rupture strength and creep limit

Creep properties of 1.4835 at elevated temperature, MPa
Property600 °C700 °C 800 °C900 °C1000 °C
Creep rupture Rz/1 000h238105502412
Creep rupture Rz/10 000h1576327137
Creep rupture Rz/100 000h88351584
Creep limit R1/1 000h170663115.58
Creep limit R1/10 000h1264519105
Creep limit R1/100 000h80261163

Heat Treatment and Hot Working

Heat treatment parameters
OperationTemperatureTimeCooling
Softening, solution annealing1020-1120 °C5-20 minRapid, in air or water
Stress relief annealing850-950 °Cunder 30 minFast in air
Hot forging, thermo-mechanical working900-1150 °C-Per forging schedule
Hot bending850-1100 °C--

Note that 850 to 950 °C is a stress relief treatment only. It does not replace solution annealing at 1020 to 1120 °C, which is the treatment that restores the austenitic structure after hot forging. Components that have been cold bent and will run above 800 °C are normally annealed afterwards.

Forming, Welding and Machining

Forming

  • Cold formed in the same way as other high-alloy austenitic steels.
  • The nitrogen content means higher forming forces than 1.4841 / X15CrNiSi25-21.
  • Springback is pronounced, so allow compensation in the tooling.
  • Ductility is considerably better than the ferritic heat-resisting grades.

Welding

  • Welded by SMAW, GTAW, plasma arc and submerged arc processes.
  • Use low heat input and filler metal of matching EN 1.4835 type.
  • TIG and MIG give the best creep performance at temperature.
  • Hardenable by cold work only, not by heat treatment.

Machining

  • Work-hardening austenitic grade. Use sharp tooling, rigid setups and positive feed, and avoid dwelling.
  • Low sulphur content means no free-machining additives, so plan on reduced speeds.
  • Forgings can be supplied rough machined or finish machined to drawing.

Behaviour in service atmospheres

  • Chromium oxide scale gives oxidation resistance reported to 1150 °C in air.
  • Good in carburising and nitriding atmospheres, though AISI 310 and 314 (1.4841) perform better.
  • Resistance to sulphur compounds approaches the ferritic grades 1.4742 and 1.4762.
  • Water vapour degrades oxidation resistance and can cut maximum service temperature by up to 100 °C.

Comparison With Neighbouring Grades

Reported performance against other heat-resisting grades
ComparisonReported behaviour
Against 309 stainlessRolled Alloys reports oxidation resistance of RA 253 MA good to 2000 °F (1093 °C), superior to 309, with creep strength twice that of 309 and 310 above 1600 °F.
Against 310 stainlessOxidation performance comparable to 310. In strongly carburising atmospheres, 310 and 314 remain the better choice.
Against X15CrNiSi25-21 (1.4841)Lower chromium and nickel content, which reduces cost, and performance that often allows smaller sections and thinner walls.
Against 1.4818 (153 MA, S30415)A different and leaner 19Cr-10Ni cerium grade. Do not substitute one for the other without review.

Applications

Published application lists for X9CrNiSiNCe21-11-2 / 1.4835 / 253MA cover high-temperature plant rather than wet corrosion service. They include combustion chambers, recuperators and heat exchangers, heat treatment furnace tubes and fixtures, radiant and radiator tubes, air heating tubes in sulphuric acid gas converters, thermocouple tubes, burner components, exhaust manifolds, turbine and fan rotors, impact separators, ash hopper covers, furnace refractory anchors, circulating fluidised bed boiler parts, pipe hooks and tubular guards, glass foundry moulds, styrene reactor and convection tubes, and equipment for the steelworks, glass and cement industries.

Forged shapes produced against those duties include seamless rolled rings and casing rings, flanges and tube sheets, shafts and spindles, discs and blanks, sleeves and bushings, hollow forged tubes, nozzles, and valve bodies, seat rings and stems.

For duties outside this range, in particular aqueous or acid corrosion service, send the operating conditions with the enquiry. A duplex, 6Mo or nickel alloy from the stainless steel or nickel alloy range may be the correct material instead.

Manufacturing and Quality Control

Melting and forging

  • EAF and VOD refining, with ESR remelting where cleanliness is critical.
  • Open-die forging and seamless ring rolling.
  • Forging range 900 to 1150 °C with controlled reduction ratio.
  • Solution annealing after forging at 1020 to 1120 °C.

Testing and documentation

  • Ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388.
  • Chemical analysis, tensile, impact and hardness testing.
  • Intergranular corrosion and grain size testing on request.
  • EN 10204 3.1 certificates, or 3.2 with third party witness.

Frequently Asked Questions

Is X8CrNiSiN21-11 the same material as 253MA?

X8CrNiSiN21-11 appears in published cross reference lists as an alternative designation within the X9CrNiSiNCe21-11-2 / 1.4835 / 253MA / UNS S30815 family, alongside 1.4893, SS 2368 and ISO X7CrNiSiNCe21-11. Cross references of this kind are indicative rather than contractual, so confirm the exact specification required on the purchase order and the material will be certified to it.

What is the maximum service temperature?

Atlas Steels and AZoM state that 253MA resists oxidation at temperatures up to 1150 °C, and the most suitable structural range is quoted as 850 to 1100 °C. Water vapour in the atmosphere can lower that ceiling by up to 100 °C because it accelerates breakdown of the protective oxide.

Which heat treatment should be specified on the order?

For forgings, specify solution annealing at 1020 to 1120 °C with rapid cooling in air or water, the +AT condition. Add stress relief at 850 to 950 °C only where residual stress from machining or welding has to be reduced. It is an additional step, not a substitute.

What sizes and shapes can be forged?

Rolled rings, flanges, discs, bars, sleeves, shafts, tube sheets and hollow tubes are produced to customer drawing. Send the drawing or finished dimensions with tolerances, quantity, test requirements and certificate level to sales@steelforgepieces.com and feasibility, weight and lead time will be confirmed.

Is third party certification available?

Yes. Material is supplied with EN 10204 3.1 certification as standard. EN 10204 3.2 with inspection by a third party body such as TUV, SGS, BV or Lloyd's can be arranged when it is specified at order stage.

Request a Quotation

Jiangyin Jiangnan Metal Co., Ltd., Open-Die Forging Factory
Address: No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel: +86-189-2135-9659
Email: sales@steelforgepieces.com

Pricing is quoted per drawing. For an accurate price by return, please include the grade and standard, a drawing or rough dimensions, the quantity, the required heat treatment condition, NDT requirements and the certificate level.

Email your drawing

Standards and Data Sources

  • EN 10095, Heat Resisting Steels and Nickel Alloys. EN 10088-1, List of Stainless Steels.
  • Virgamet grade datasheet for X9CrNiSiNCe21-11-2 / 1.4835 / 253MA: composition cross reference, creep data, heat treatment and applications.
  • Atlas Steels and AZoM grade data sheets for Stainless Steel 253MA (UNS S30815): oxidation resistance to 1150 °C.
  • Rolled Alloys, RA 253 MA versus 309/310: comparative oxidation and creep performance.
  • Fushun Special Steel datasheet for 1.4835 / X9CrNiSiNCe21-11-2: service range and equivalent designations.

Published property values are indicative. Contractual values are those stated on the material certificate. Page last reviewed 11 October 2026.